Skip to main content
All case studies

Custom machined bearing cover

A 1.35 m cast-iron cover rebuilt from a cracked sample. Casting defects and annealing distortion were the two things to hold; the face and spigot were checked to the German assembly tolerance.

+86 187 3757 7920
Large ring-shaped HT200 bearing end cover with a yellow-primed flange, photographed on a concrete floor.

Job facts

Industry
Mining
Part
Rolling bearing end cover, oil lubricated
Quantity
1 set (2 pieces)
Net weight
1.5 t per set
Main dimensions
Ø1350 mm × H315 mm
Material
HT200
Heat treatment
Stress-relief annealing
Lead time
8 weeks
Delivered
June 2026
Destination
Germany
Customer
Anonymous

Bearing end cover for a German mine

The old cover had cracked after years of alternating load, and there was no complete original drawing. The part is large in diameter, the casting has uneven wall thickness, and both casting and annealing tend to distort it; several suppliers could not hold the flatness on a part this size. The customer also required strict non-destructive testing, and the lead time was tight. The hardest part was controlling casting defects and heat-treatment distortion in a large HT200 casting while holding the face and spigot inside the German assembly tolerance.

We measured the damaged sample and rebuilt the model, then set the route: casting, rough machining, annealing, finish machining. In the foundry the gating and risering were changed to reduce shrinkage porosity. Annealing was run with controlled heating, holding and cooling rates to relieve residual stress before machining. A second inspection after rough turning removed defective material early; finish turning and milling followed. Because the old cover had cracked, the job focused on casting defects and residual stress.

How it was made

Send a drawing
  1. Casting

    A pattern was made from the measured sample; HT200 poured with gating and risering set to reduce shrinkage porosity.

  2. Annealing

    Stress-relief anneal with controlled heating, holding and cooling so the part would not move after machining.

  3. First inspection

    MT on the accessible surfaces to catch cracks before any value was added.

  4. Rough turning

    Stock removed evenly, with enough left for the finish cut after stress relief.

  5. Second inspection

    A second MT pass after rough turning removed defective material before finish machining.

  6. Finish turning

    Spigot and faces cut to the drawing tolerance; flatness checked on the plate.

  7. Finish milling

    Mounting features milled and the finished part checked against the drawing.

Inspection and result

The casting passed MT magnetic-particle inspection with no surface cracks. Critical spigot and face dimensions were all inside the drawing tolerance, and flatness met the assembly requirement. After installation in Germany the cover ran without leakage or distortion; the customer accepted the casting quality and dimensional control and kept us in mind for repeat work.

Surface inspection
MT, no surface cracks
Critical dimensions
Spigot and face inside drawing tolerance
Flatness
Meets the assembly requirement
After installation
No leakage or distortion; customer accepted the part

Packing and delivery

Solid-wood crate with rust-preventive oil and a steel frame to stop movement in transit; sea freight to a German port, protected against moisture and impact for the whole voyage.

Have a part like this?

Send the drawing, or the worn sample. We reply with what we can measure, the material questions we still need answered, and a date.

Send a drawing