Skip to main content
All case studies

Custom split girth gear

A 5.2 m split girth gear rebuilt from a worn and broken sample. Heat-treatment distortion and the joint faces were the two things to hold; the gear was pre-assembled in the works.

+86 187 3757 7920
Two red-primed halves of a large split girth gear on the workshop floor.

Job facts

Industry
Cement
Part
Rotary kiln girth gear (split girth gear)
Quantity
1 set (2 pieces)
Net weight
20 t per set
Main dimensions
Ø5200 mm × 450 mm face width
Material
ZG35, reproduced to the old part
Heat treatment
Quench and temper + tooth-flank hardening
Lead time
8 weeks (expedited)
Delivered
March 2026
Destination
Kazakhstan
Customer
A cement plant (name withheld)

Split girth gear for a cement plant in Kazakhstan

The old gear had worn and broken, and there was no original drawing. At 5.2 m it is beyond the machine capacity of many Chinese shops. The customer needed the spare to restart the kiln, so the schedule was short. The hard part was controlling heat-treatment distortion on a large split ring and holding the joint faces accurate enough for assembly on site.

We reverse-engineered the old gear and rebuilt the drawing, keeping the old material ZG35 rather than substituting a grade. The route was casting, post-cast normalising and annealing, quench and temper, joint-face milling, bolting the halves, rough turning, finish turning of the datum, hobbing, tooth-flank hardening and final turning of the spigot. Heat treatment was controlled and machining allowance was left to take out distortion. The halves were pre-assembled in the works so the site joint would close.

How it was made

Send a drawing
  1. Casting

    Two ZG35 halves cast to the rebuilt drawing.

  2. Post-cast normalising

    Cast stress released before the ring is machined.

  3. Quench and temper

    Blank quenched and tempered to the drawing core hardness.

  4. Joint-face milling

    Joint faces milled after heat treatment so the halves close without a gap.

  5. Bolting the halves

    The two halves are joined and match-marked as one ring.

  6. Rough turning

    The joined ring is roughed with allowance for the heat-treatment move.

  7. Finish turning (datum)

    Bore and face finished to give the hobbing a true datum.

  8. Hobbing

    Large-module teeth cut on the gear hobbing machine.

  9. Tooth-flank hardening

    Flanks hardened to the drawing hardness.

  10. Finish turning (spigot)

    Spigot and faces cleaned up after hardening.

  11. Inspection

    Hardness, UT and tooth accuracy checked before dispatch.

Inspection and result

Tooth-flank hardness met the drawing HRC; UT passed; tooth accuracy met the customer grade 8 acceptance. Critical dimensions were inside tolerance. The gear ran smoothly on site, with vibration and temperature readings normal, and the customer placed further orders.

Tooth-flank hardness
Meets the drawing HRC
Internal soundness
UT passed
Tooth accuracy
Grade 8, customer acceptance
On site
Vibration and temperature normal

Packing and delivery

Steel frame and rust-preventive oil; each half packed separately. Road to port, then a flat rack for over-width cargo to Kazakhstan.

Have a part like this?

Send the drawing, or the worn sample. We reply with what we can measure, the material questions we still need answered, and a date.

Send a drawing